P.K. Hu, H. Wu, R. Wang, C.H. Zhang, S. Zhang, C.L. Wu, F.P. Huo, H.T. Chen
{"title":"镍含量对激光熔覆 Cu-10Sn 涂层电化学腐蚀和摩擦学行为的影响","authors":"P.K. Hu, H. Wu, R. Wang, C.H. Zhang, S. Zhang, C.L. Wu, F.P. Huo, H.T. Chen","doi":"10.1016/j.mtcomm.2024.110370","DOIUrl":null,"url":null,"abstract":"In this work, Cu-10Sn-Ni ( = 0, 3, 6, 9, and 12 wt%) alloy coatings were prepared using laser cladding technology. The influence of Ni content on the phase composition, microstructure, crystallographic characteristics, microhardness, electrochemical corrosion, dry sliding wear and corrosive wear behavior of the coatings were studied. The results indicated that the coatings formed good metallurgical bond with the substrate. The coatings were composed primarily of the α-Cu matrix and small γ precipitates. The Ni element effectively reduced component segregation, and with the increased of Ni content, the grain size in the coating was significantly refined, resulting in fine equiaxed grains. Under the effect of fine grain strengthening, the Cu-10Sn-12Ni (C12NS) coating achieved a higher microhardness of approximately 222.9 ± 5.3 HV. In the electrochemical corrosion test, the increased in the number of grain boundaries significantly reduced the corrosion resistance of the Cu-10Sn-Ni coatings. The Cu-10Sn-6Ni (C6NS) coating exhibited excellent corrosion resistance, with an of only 1.37 μA/cm. The results of the dry sliding wear test showed that under the influence of the hardness gradient between the hard precipitate phase and the soft matrix of the coating, the C6NS coating achieved satisfactory wear resistance with a specific wear rate of 3.30 × 10 μm/Nm. Meanwhile, due to the good corrosive resistance, the C6NS coating showed the best tribological performance in 3.5 wt% NaCl environment, and the specific wear rate was 1.58 × 10 μm/Nm.","PeriodicalId":18477,"journal":{"name":"Materials Today Communications","volume":"105 1","pages":""},"PeriodicalIF":3.7000,"publicationDate":"2024-09-07","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Influence of Ni content on electrochemical corrosion and tribological behavior of Cu-10Sn coatings by laser cladding\",\"authors\":\"P.K. Hu, H. Wu, R. Wang, C.H. Zhang, S. Zhang, C.L. Wu, F.P. Huo, H.T. Chen\",\"doi\":\"10.1016/j.mtcomm.2024.110370\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"In this work, Cu-10Sn-Ni ( = 0, 3, 6, 9, and 12 wt%) alloy coatings were prepared using laser cladding technology. The influence of Ni content on the phase composition, microstructure, crystallographic characteristics, microhardness, electrochemical corrosion, dry sliding wear and corrosive wear behavior of the coatings were studied. The results indicated that the coatings formed good metallurgical bond with the substrate. The coatings were composed primarily of the α-Cu matrix and small γ precipitates. The Ni element effectively reduced component segregation, and with the increased of Ni content, the grain size in the coating was significantly refined, resulting in fine equiaxed grains. Under the effect of fine grain strengthening, the Cu-10Sn-12Ni (C12NS) coating achieved a higher microhardness of approximately 222.9 ± 5.3 HV. In the electrochemical corrosion test, the increased in the number of grain boundaries significantly reduced the corrosion resistance of the Cu-10Sn-Ni coatings. The Cu-10Sn-6Ni (C6NS) coating exhibited excellent corrosion resistance, with an of only 1.37 μA/cm. The results of the dry sliding wear test showed that under the influence of the hardness gradient between the hard precipitate phase and the soft matrix of the coating, the C6NS coating achieved satisfactory wear resistance with a specific wear rate of 3.30 × 10 μm/Nm. Meanwhile, due to the good corrosive resistance, the C6NS coating showed the best tribological performance in 3.5 wt% NaCl environment, and the specific wear rate was 1.58 × 10 μm/Nm.\",\"PeriodicalId\":18477,\"journal\":{\"name\":\"Materials Today Communications\",\"volume\":\"105 1\",\"pages\":\"\"},\"PeriodicalIF\":3.7000,\"publicationDate\":\"2024-09-07\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Materials Today Communications\",\"FirstCategoryId\":\"88\",\"ListUrlMain\":\"https://doi.org/10.1016/j.mtcomm.2024.110370\",\"RegionNum\":3,\"RegionCategory\":\"材料科学\",\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q2\",\"JCRName\":\"MATERIALS SCIENCE, MULTIDISCIPLINARY\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Materials Today Communications","FirstCategoryId":"88","ListUrlMain":"https://doi.org/10.1016/j.mtcomm.2024.110370","RegionNum":3,"RegionCategory":"材料科学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q2","JCRName":"MATERIALS SCIENCE, MULTIDISCIPLINARY","Score":null,"Total":0}
Influence of Ni content on electrochemical corrosion and tribological behavior of Cu-10Sn coatings by laser cladding
In this work, Cu-10Sn-Ni ( = 0, 3, 6, 9, and 12 wt%) alloy coatings were prepared using laser cladding technology. The influence of Ni content on the phase composition, microstructure, crystallographic characteristics, microhardness, electrochemical corrosion, dry sliding wear and corrosive wear behavior of the coatings were studied. The results indicated that the coatings formed good metallurgical bond with the substrate. The coatings were composed primarily of the α-Cu matrix and small γ precipitates. The Ni element effectively reduced component segregation, and with the increased of Ni content, the grain size in the coating was significantly refined, resulting in fine equiaxed grains. Under the effect of fine grain strengthening, the Cu-10Sn-12Ni (C12NS) coating achieved a higher microhardness of approximately 222.9 ± 5.3 HV. In the electrochemical corrosion test, the increased in the number of grain boundaries significantly reduced the corrosion resistance of the Cu-10Sn-Ni coatings. The Cu-10Sn-6Ni (C6NS) coating exhibited excellent corrosion resistance, with an of only 1.37 μA/cm. The results of the dry sliding wear test showed that under the influence of the hardness gradient between the hard precipitate phase and the soft matrix of the coating, the C6NS coating achieved satisfactory wear resistance with a specific wear rate of 3.30 × 10 μm/Nm. Meanwhile, due to the good corrosive resistance, the C6NS coating showed the best tribological performance in 3.5 wt% NaCl environment, and the specific wear rate was 1.58 × 10 μm/Nm.
期刊介绍:
Materials Today Communications is a primary research journal covering all areas of materials science. The journal offers the materials community an innovative, efficient and flexible route for the publication of original research which has not found the right home on first submission.