{"title":"骨钻骨折","authors":"F. Naumann, F. Spies","doi":"10.31399/asm.fach.med.c9001187","DOIUrl":null,"url":null,"abstract":"\n A stainless tool steel bone drill broke during an operation on a patient and was examined. It showed two fatigue fractures, one of which had started from a sharp-edged, coarsely milled slot (fracture A1), and the other from a point on the outer sheath surface which was not subjected to particularly high stresses (fracture A2). Fatigue fracture A1 resulted from the stress concentration built up at this point as a result of the sharp edges and the coarse machining grooves. The remains of a number, which had been inscribed with an electrical engraving tool for identification purposes, were found at the point of origin of fracture A2. The material had been heated to the melting point during the engraving of the number, and multiple cracking occurred during cooling. One of these cracks led to the development of fatigue fracture A2.","PeriodicalId":125471,"journal":{"name":"ASM Failure Analysis Case Histories: Medical and Biomedical Devices","volume":"193 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"2019-06-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Fracture of a Bone Drill\",\"authors\":\"F. Naumann, F. Spies\",\"doi\":\"10.31399/asm.fach.med.c9001187\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"\\n A stainless tool steel bone drill broke during an operation on a patient and was examined. It showed two fatigue fractures, one of which had started from a sharp-edged, coarsely milled slot (fracture A1), and the other from a point on the outer sheath surface which was not subjected to particularly high stresses (fracture A2). Fatigue fracture A1 resulted from the stress concentration built up at this point as a result of the sharp edges and the coarse machining grooves. The remains of a number, which had been inscribed with an electrical engraving tool for identification purposes, were found at the point of origin of fracture A2. The material had been heated to the melting point during the engraving of the number, and multiple cracking occurred during cooling. One of these cracks led to the development of fatigue fracture A2.\",\"PeriodicalId\":125471,\"journal\":{\"name\":\"ASM Failure Analysis Case Histories: Medical and Biomedical Devices\",\"volume\":\"193 1\",\"pages\":\"0\"},\"PeriodicalIF\":0.0000,\"publicationDate\":\"2019-06-01\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"ASM Failure Analysis Case Histories: Medical and Biomedical Devices\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.31399/asm.fach.med.c9001187\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"ASM Failure Analysis Case Histories: Medical and Biomedical Devices","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.31399/asm.fach.med.c9001187","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 0

摘要

一个不锈钢工具钢骨钻在一个病人的手术中断裂并被检查。它显示了两个疲劳断裂,其中一个是从一个锋利的,粗糙的铣削槽开始的(断口A1),另一个是从外护套表面的一个点开始的,这个点没有受到特别高的应力(断口A2)。疲劳断裂A1是由于锋利的边缘和粗糙的加工槽在这一点上形成的应力集中造成的。在A2断口的起源处发现了一个数字的残骸,这个数字是用电子雕刻工具刻上的,用于识别目的。在雕刻数字时,材料被加热到熔点,在冷却过程中出现多次开裂。其中一个裂纹导致疲劳断裂A2的发展。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
Fracture of a Bone Drill
A stainless tool steel bone drill broke during an operation on a patient and was examined. It showed two fatigue fractures, one of which had started from a sharp-edged, coarsely milled slot (fracture A1), and the other from a point on the outer sheath surface which was not subjected to particularly high stresses (fracture A2). Fatigue fracture A1 resulted from the stress concentration built up at this point as a result of the sharp edges and the coarse machining grooves. The remains of a number, which had been inscribed with an electrical engraving tool for identification purposes, were found at the point of origin of fracture A2. The material had been heated to the melting point during the engraving of the number, and multiple cracking occurred during cooling. One of these cracks led to the development of fatigue fracture A2.
求助全文
通过发布文献求助,成功后即可免费获取论文全文。 去求助
来源期刊
自引率
0.00%
发文量
0
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
确定
请完成安全验证×
copy
已复制链接
快去分享给好友吧!
我知道了
右上角分享
点击右上角分享
0
联系我们:info@booksci.cn Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。 Copyright © 2023 布克学术 All rights reserved.
京ICP备2023020795号-1
ghs 京公网安备 11010802042870号
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术官方微信