微孔隙引起灰铸铁缸盖开裂

{"title":"微孔隙引起灰铸铁缸盖开裂","authors":"","doi":"10.31399/asm.fach.auto.c0089526","DOIUrl":null,"url":null,"abstract":"\n A gray iron cylinder head cracked after approximately 16,000 km of service. The head was cracked on the rocker arm pan rail next to the No. 3 intake port and extended into the water jacket on the rocker-arm side of the head. Microporosity was revealed in the crack in the sections taken from the water jacket next to the plug and the area next to the No. 3 intake port. A wave of microporosity travels midway between the inner and outer surfaces of the casting was observed and was concluded to have caused the cracking. The reasons and remedies for shrinkage porosity were discussed. Controlled pouring temperatures, improved design and use of chills were recommended to avoid the casting defects.","PeriodicalId":235345,"journal":{"name":"ASM Failure Analysis Case Histories: Automobiles and Trucks","volume":"115 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"2019-06-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Cracking in a Gray-Iron Cylinder Head Caused by Microporosity\",\"authors\":\"\",\"doi\":\"10.31399/asm.fach.auto.c0089526\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"\\n A gray iron cylinder head cracked after approximately 16,000 km of service. The head was cracked on the rocker arm pan rail next to the No. 3 intake port and extended into the water jacket on the rocker-arm side of the head. Microporosity was revealed in the crack in the sections taken from the water jacket next to the plug and the area next to the No. 3 intake port. A wave of microporosity travels midway between the inner and outer surfaces of the casting was observed and was concluded to have caused the cracking. The reasons and remedies for shrinkage porosity were discussed. Controlled pouring temperatures, improved design and use of chills were recommended to avoid the casting defects.\",\"PeriodicalId\":235345,\"journal\":{\"name\":\"ASM Failure Analysis Case Histories: Automobiles and Trucks\",\"volume\":\"115 1\",\"pages\":\"0\"},\"PeriodicalIF\":0.0000,\"publicationDate\":\"2019-06-01\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"ASM Failure Analysis Case Histories: Automobiles and Trucks\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.31399/asm.fach.auto.c0089526\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"ASM Failure Analysis Case Histories: Automobiles and Trucks","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.31399/asm.fach.auto.c0089526","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 0

摘要

一个灰铁气缸盖在使用了大约16000公里后出现了裂纹。机头在靠近3号进气口的摇臂盘轨上开裂,并延伸到机头摇臂侧的水套内。在靠近堵头的水套和靠近3号进气口的区域的裂缝处发现了微孔隙。在铸件内外表面之间观察到微孔隙波,并得出导致裂纹的结论。讨论了缩孔缩松产生的原因及补救措施。建议控制浇注温度,改进冷冻机的设计和使用,以避免铸件缺陷。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
Cracking in a Gray-Iron Cylinder Head Caused by Microporosity
A gray iron cylinder head cracked after approximately 16,000 km of service. The head was cracked on the rocker arm pan rail next to the No. 3 intake port and extended into the water jacket on the rocker-arm side of the head. Microporosity was revealed in the crack in the sections taken from the water jacket next to the plug and the area next to the No. 3 intake port. A wave of microporosity travels midway between the inner and outer surfaces of the casting was observed and was concluded to have caused the cracking. The reasons and remedies for shrinkage porosity were discussed. Controlled pouring temperatures, improved design and use of chills were recommended to avoid the casting defects.
求助全文
通过发布文献求助,成功后即可免费获取论文全文。 去求助
来源期刊
自引率
0.00%
发文量
0
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
确定
请完成安全验证×
copy
已复制链接
快去分享给好友吧!
我知道了
右上角分享
点击右上角分享
0
联系我们:info@booksci.cn Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。 Copyright © 2023 布克学术 All rights reserved.
京ICP备2023020795号-1
ghs 京公网安备 11010802042870号
Book学术文献互助
Book学术文献互助群
群 号:604180095
Book学术官方微信