Ekaterina Filimonova, Thomas Bergmann, Shanyu Zhao, Valery A. Dyatlov, Wim J. Malfait, Tingting Wu
{"title":"Effect of polymer concentration and cross-linking density on the microstructure and properties of polyimide aerogels","authors":"Ekaterina Filimonova, Thomas Bergmann, Shanyu Zhao, Valery A. Dyatlov, Wim J. Malfait, Tingting Wu","doi":"10.1007/s10971-024-06390-0","DOIUrl":null,"url":null,"abstract":"<div><p>Polyimide aerogels display excellent mechanical strength, high thermal stability, low thermal conductivity, and outstanding dielectric properties. Typically, the synthesis of polyimide aerogels involves the polycondensation of dianhydride and diamine into poly(amic acid) (PAA) oligomers, which are then cross-linked and chemically imidized into polyimide. The stoichiometry of dianhydride and diamine determines the number of repeat units and length of the PAA oligomers, which in turn determines the cross-linking density. Despite the critical role of polymer concentration and number of repeating units in determining the microstructure and properties of polyimide aerogels, few detailed studies exist on these two parameters. Here, we synthesized and characterized 16 polyimide aerogel formulations from the common monomers biphenyl-3,3′,4,4′-tetracarboxylic dianhydride (BPDA) and 4,4′-oxydianiline (ODA), with different repeat units (<i>n</i> = 5, 15, 30, 45) and total polymer concentrations (4, 7, 10, 13 wt%). An increased polymer concentration accelerated gelation and enhanced the mechanical performance of aerogels, but surprisingly, it also led to higher volumetric shrinkage during aging, solvent exchange, and supercritical drying (SCD). Specific surface areas (SSAs) reached a maximum at intermediate polymer concentrations. A shorter oligomer chain length, i.e., a higher cross-linking density, led to moderately higher SSAs (between 320 and 400 m<sup>2</sup>/g) and reduced shrinkage, resulting in lower densities for a given polymer concentration. The density dependence of the thermal conductivity exhibits a pronounced <i>U</i>-shaped curve with a minimum in thermal conductivity of 21–23 mW/(m·K) between 0.080 and 0.120 g/cm<sup>3</sup>, with somewhat lower values for more highly cross-linked aerogels. This systematic study of polyimide aerogels forms the basis for designing polyimide aerogels with tailored properties for targeted applications.</p><h3>Graphical Abstract</h3><div><figure><div><div><picture><source><img></source></picture></div></div></figure></div></div>","PeriodicalId":664,"journal":{"name":"Journal of Sol-Gel Science and Technology","volume":null,"pages":null},"PeriodicalIF":2.3000,"publicationDate":"2024-05-10","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"https://link.springer.com/content/pdf/10.1007/s10971-024-06390-0.pdf","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"Journal of Sol-Gel Science and Technology","FirstCategoryId":"88","ListUrlMain":"https://link.springer.com/article/10.1007/s10971-024-06390-0","RegionNum":4,"RegionCategory":"材料科学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q2","JCRName":"MATERIALS SCIENCE, CERAMICS","Score":null,"Total":0}
引用次数: 0
Abstract
Polyimide aerogels display excellent mechanical strength, high thermal stability, low thermal conductivity, and outstanding dielectric properties. Typically, the synthesis of polyimide aerogels involves the polycondensation of dianhydride and diamine into poly(amic acid) (PAA) oligomers, which are then cross-linked and chemically imidized into polyimide. The stoichiometry of dianhydride and diamine determines the number of repeat units and length of the PAA oligomers, which in turn determines the cross-linking density. Despite the critical role of polymer concentration and number of repeating units in determining the microstructure and properties of polyimide aerogels, few detailed studies exist on these two parameters. Here, we synthesized and characterized 16 polyimide aerogel formulations from the common monomers biphenyl-3,3′,4,4′-tetracarboxylic dianhydride (BPDA) and 4,4′-oxydianiline (ODA), with different repeat units (n = 5, 15, 30, 45) and total polymer concentrations (4, 7, 10, 13 wt%). An increased polymer concentration accelerated gelation and enhanced the mechanical performance of aerogels, but surprisingly, it also led to higher volumetric shrinkage during aging, solvent exchange, and supercritical drying (SCD). Specific surface areas (SSAs) reached a maximum at intermediate polymer concentrations. A shorter oligomer chain length, i.e., a higher cross-linking density, led to moderately higher SSAs (between 320 and 400 m2/g) and reduced shrinkage, resulting in lower densities for a given polymer concentration. The density dependence of the thermal conductivity exhibits a pronounced U-shaped curve with a minimum in thermal conductivity of 21–23 mW/(m·K) between 0.080 and 0.120 g/cm3, with somewhat lower values for more highly cross-linked aerogels. This systematic study of polyimide aerogels forms the basis for designing polyimide aerogels with tailored properties for targeted applications.
期刊介绍:
The primary objective of the Journal of Sol-Gel Science and Technology (JSST), the official journal of the International Sol-Gel Society, is to provide an international forum for the dissemination of scientific, technological, and general knowledge about materials processed by chemical nanotechnologies known as the "sol-gel" process. The materials of interest include gels, gel-derived glasses, ceramics in form of nano- and micro-powders, bulk, fibres, thin films and coatings as well as more recent materials such as hybrid organic-inorganic materials and composites. Such materials exhibit a wide range of optical, electronic, magnetic, chemical, environmental, and biomedical properties and functionalities. Methods for producing sol-gel-derived materials and the industrial uses of these materials are also of great interest.