15-7Mo钢热处理后焊缝的组织和织构

A. Ziewiec, A. Zielińska-Lipiec, M. Witkowska
{"title":"15-7Mo钢热处理后焊缝的组织和织构","authors":"A. Ziewiec, A. Zielińska-Lipiec, M. Witkowska","doi":"10.7494/mafe.2016.42.4.225","DOIUrl":null,"url":null,"abstract":"This paper presents the results of determining the effect of heat treatment after welding X8CrNiMoAl15-7-2 steel (commercial name: PH 15-7Mo steel) on the microstructure and texture of the welds. XRD studies showed the presence of the two phases in the welds of 15-7Mo steel; i.e., δ ferrite and austenite. Annealing at a temperature of 400°C/1 h and 550°C/1 h results in changes of the intensities for individual peaks derived from austenite and ferrite. Microstructure investigations carried out by LM and TEM indicated that the austenite and δ ferrite coexist in the microstructure of 15-7Mo steel in as-welded condition. Annealing at a temperature range of between 400–620°C after welding causes small changes in the microstructure. The hardness of the welds after annealing in that temperature range increases.","PeriodicalId":18751,"journal":{"name":"Metallurgy and Foundry Engineering","volume":"25 1","pages":"225"},"PeriodicalIF":0.0000,"publicationDate":"2016-01-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"MICROSTRUCTURE AND TEXTURE WELDS OF 15-7Mo STEEL AFTER HEAT TREATMENT\",\"authors\":\"A. Ziewiec, A. Zielińska-Lipiec, M. Witkowska\",\"doi\":\"10.7494/mafe.2016.42.4.225\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"This paper presents the results of determining the effect of heat treatment after welding X8CrNiMoAl15-7-2 steel (commercial name: PH 15-7Mo steel) on the microstructure and texture of the welds. XRD studies showed the presence of the two phases in the welds of 15-7Mo steel; i.e., δ ferrite and austenite. Annealing at a temperature of 400°C/1 h and 550°C/1 h results in changes of the intensities for individual peaks derived from austenite and ferrite. Microstructure investigations carried out by LM and TEM indicated that the austenite and δ ferrite coexist in the microstructure of 15-7Mo steel in as-welded condition. Annealing at a temperature range of between 400–620°C after welding causes small changes in the microstructure. The hardness of the welds after annealing in that temperature range increases.\",\"PeriodicalId\":18751,\"journal\":{\"name\":\"Metallurgy and Foundry Engineering\",\"volume\":\"25 1\",\"pages\":\"225\"},\"PeriodicalIF\":0.0000,\"publicationDate\":\"2016-01-01\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Metallurgy and Foundry Engineering\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.7494/mafe.2016.42.4.225\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Metallurgy and Foundry Engineering","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.7494/mafe.2016.42.4.225","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 0

摘要

本文介绍了X8CrNiMoAl15-7-2钢(商品名称:ph15 - 7mo钢)焊接后热处理对焊缝组织和织构影响的测定结果。XRD研究表明,15-7Mo钢焊缝中存在两相;即δ铁素体和奥氏体。在400°C/1 h和550°C/1 h的退火温度下,奥氏体和铁素体产生的单个峰的强度发生变化。LM和TEM分析表明,15-7Mo钢在焊接状态下的组织中存在奥氏体和δ铁素体。焊接后在400-620℃的温度范围内退火,导致微观组织发生微小变化。在该温度范围内退火后,焊缝的硬度增加。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
MICROSTRUCTURE AND TEXTURE WELDS OF 15-7Mo STEEL AFTER HEAT TREATMENT
This paper presents the results of determining the effect of heat treatment after welding X8CrNiMoAl15-7-2 steel (commercial name: PH 15-7Mo steel) on the microstructure and texture of the welds. XRD studies showed the presence of the two phases in the welds of 15-7Mo steel; i.e., δ ferrite and austenite. Annealing at a temperature of 400°C/1 h and 550°C/1 h results in changes of the intensities for individual peaks derived from austenite and ferrite. Microstructure investigations carried out by LM and TEM indicated that the austenite and δ ferrite coexist in the microstructure of 15-7Mo steel in as-welded condition. Annealing at a temperature range of between 400–620°C after welding causes small changes in the microstructure. The hardness of the welds after annealing in that temperature range increases.
求助全文
通过发布文献求助,成功后即可免费获取论文全文。 去求助
来源期刊
自引率
0.00%
发文量
0
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
确定
请完成安全验证×
copy
已复制链接
快去分享给好友吧!
我知道了
右上角分享
点击右上角分享
0
联系我们:info@booksci.cn Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。 Copyright © 2023 布克学术 All rights reserved.
京ICP备2023020795号-1
ghs 京公网安备 11010802042870号
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术官方微信