{"title":"重型货运列车用铁路轨道故障研究","authors":"Y.D. Li ,&nbsp;C.B. Liu ,&nbsp;N. Xu ,&nbsp;X.F. Wu ,&nbsp;W.M. Guo ,&nbsp;J.B. Shi","doi":"10.1016/j.csefa.2013.09.003","DOIUrl":null,"url":null,"abstract":"<div><p>In this case study, a failed railway rail which was used for heavy cargo trains was investigated in order to find out its root cause. The macroscopic beach marks and microscopic fatigue striations were not observed by macro and microscopic observations. The chevron patterns were observed by macro observations. The crack origin was at the tip of chevron patterns. The fan-shaped patterns, cleavage step and the river patterns were observed at the crack origin, which demonstrated the feature of cleavage fracture. The metallurgical structures at the crack origin were pearlite and ferrite networks. The crack is supposed to be initiated from the weaker ferrite networks. Given all of that, the failed railway rail is considered to be caused by overload. It is of great importance to improve the welding technology, and control the load of train in order to prevent similar failure in future.</p></div>","PeriodicalId":91224,"journal":{"name":"Case studies in engineering failure analysis","volume":"1 4","pages":"Pages 243-248"},"PeriodicalIF":0.0000,"publicationDate":"2013-10-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"https://sci-hub-pdf.com/10.1016/j.csefa.2013.09.003","citationCount":"20","resultStr":"{\"title\":\"A failure study of the railway rail serviced for heavy cargo trains\",\"authors\":\"Y.D. Li ,&nbsp;C.B. Liu ,&nbsp;N. Xu ,&nbsp;X.F. Wu ,&nbsp;W.M. Guo ,&nbsp;J.B. Shi\",\"doi\":\"10.1016/j.csefa.2013.09.003\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"<div><p>In this case study, a failed railway rail which was used for heavy cargo trains was investigated in order to find out its root cause. The macroscopic beach marks and microscopic fatigue striations were not observed by macro and microscopic observations. The chevron patterns were observed by macro observations. The crack origin was at the tip of chevron patterns. The fan-shaped patterns, cleavage step and the river patterns were observed at the crack origin, which demonstrated the feature of cleavage fracture. The metallurgical structures at the crack origin were pearlite and ferrite networks. The crack is supposed to be initiated from the weaker ferrite networks. Given all of that, the failed railway rail is considered to be caused by overload. It is of great importance to improve the welding technology, and control the load of train in order to prevent similar failure in future.</p></div>\",\"PeriodicalId\":91224,\"journal\":{\"name\":\"Case studies in engineering failure analysis\",\"volume\":\"1 4\",\"pages\":\"Pages 243-248\"},\"PeriodicalIF\":0.0000,\"publicationDate\":\"2013-10-01\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"https://sci-hub-pdf.com/10.1016/j.csefa.2013.09.003\",\"citationCount\":\"20\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Case studies in engineering failure analysis\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://www.sciencedirect.com/science/article/pii/S2213290213000461\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Case studies in engineering failure analysis","FirstCategoryId":"1085","ListUrlMain":"https://www.sciencedirect.com/science/article/pii/S2213290213000461","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 20

摘要

在本案例研究中,为了找出故障的根本原因,对重型货运列车使用的铁路钢轨进行了调查。宏观和微观观察均未观察到宏观滩痕和微观疲劳条纹。通过宏观观测观察到纹样。裂纹的起源在纹样的尖端。断口处呈扇形断口、解理阶梯断口和河流断口,具有解理断口的特征。裂纹原点处的金相组织为珠光体和铁素体网络。裂纹应该是由较弱的铁氧体网络引起的。综上所述,铁路钢轨故障被认为是由超载引起的。改进焊接工艺,控制列车载荷,对今后防止类似事故的发生具有重要意义。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
A failure study of the railway rail serviced for heavy cargo trains

In this case study, a failed railway rail which was used for heavy cargo trains was investigated in order to find out its root cause. The macroscopic beach marks and microscopic fatigue striations were not observed by macro and microscopic observations. The chevron patterns were observed by macro observations. The crack origin was at the tip of chevron patterns. The fan-shaped patterns, cleavage step and the river patterns were observed at the crack origin, which demonstrated the feature of cleavage fracture. The metallurgical structures at the crack origin were pearlite and ferrite networks. The crack is supposed to be initiated from the weaker ferrite networks. Given all of that, the failed railway rail is considered to be caused by overload. It is of great importance to improve the welding technology, and control the load of train in order to prevent similar failure in future.

求助全文
通过发布文献求助,成功后即可免费获取论文全文。 去求助
来源期刊
自引率
0.00%
发文量
0
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
确定
请完成安全验证×
copy
已复制链接
快去分享给好友吧!
我知道了
右上角分享
点击右上角分享
0
联系我们:info@booksci.cn Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。 Copyright © 2023 布克学术 All rights reserved.
京ICP备2023020795号-1
ghs 京公网安备 11010802042870号
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术官方微信