{"title":"小直径圆木短柱高温后轴向力学性能。","authors":"K. He, Yu Chen, Jiayu Sun","doi":"10.37763/wr.1336-4561/65.6.925936","DOIUrl":null,"url":null,"abstract":"A total of forty-eight specimens were tested, including forty short timber columns at elevated temperatures and eight short timber columns left untreated at ambient temperature. The main parameters explored in the test include column heights (135, 180, 225 and 270 mm), elevated temperature duration (10, 20, 30, 40 and 50 min) and section form. It was found that two new failure modes were generated after the specimens exposed to the elevated temperatures: splitting failure and bottom crushing, and the ultimate bearing capacity of the specimens with bottom crushing is the lowest. The ductility of circular specimens increases with the increases of column height. When the elevated temperature duration reaches 50 min, the plasticity of the specimens basically subside. The ultimate bearing capacity of the timber columns decreases with the increase of the elevated temperature duration and the maximum reduction is about 60% percent.","PeriodicalId":23786,"journal":{"name":"Wood Research","volume":" ","pages":""},"PeriodicalIF":0.9000,"publicationDate":"2020-12-16","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Axial mechanical properties of small-diameter round timber short columns after exposure to elevated temperatures.\",\"authors\":\"K. He, Yu Chen, Jiayu Sun\",\"doi\":\"10.37763/wr.1336-4561/65.6.925936\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"A total of forty-eight specimens were tested, including forty short timber columns at elevated temperatures and eight short timber columns left untreated at ambient temperature. The main parameters explored in the test include column heights (135, 180, 225 and 270 mm), elevated temperature duration (10, 20, 30, 40 and 50 min) and section form. It was found that two new failure modes were generated after the specimens exposed to the elevated temperatures: splitting failure and bottom crushing, and the ultimate bearing capacity of the specimens with bottom crushing is the lowest. The ductility of circular specimens increases with the increases of column height. When the elevated temperature duration reaches 50 min, the plasticity of the specimens basically subside. The ultimate bearing capacity of the timber columns decreases with the increase of the elevated temperature duration and the maximum reduction is about 60% percent.\",\"PeriodicalId\":23786,\"journal\":{\"name\":\"Wood Research\",\"volume\":\" \",\"pages\":\"\"},\"PeriodicalIF\":0.9000,\"publicationDate\":\"2020-12-16\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"Wood Research\",\"FirstCategoryId\":\"88\",\"ListUrlMain\":\"https://doi.org/10.37763/wr.1336-4561/65.6.925936\",\"RegionNum\":4,\"RegionCategory\":\"农林科学\",\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"Q3\",\"JCRName\":\"MATERIALS SCIENCE, PAPER & WOOD\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"Wood Research","FirstCategoryId":"88","ListUrlMain":"https://doi.org/10.37763/wr.1336-4561/65.6.925936","RegionNum":4,"RegionCategory":"农林科学","ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q3","JCRName":"MATERIALS SCIENCE, PAPER & WOOD","Score":null,"Total":0}
Axial mechanical properties of small-diameter round timber short columns after exposure to elevated temperatures.
A total of forty-eight specimens were tested, including forty short timber columns at elevated temperatures and eight short timber columns left untreated at ambient temperature. The main parameters explored in the test include column heights (135, 180, 225 and 270 mm), elevated temperature duration (10, 20, 30, 40 and 50 min) and section form. It was found that two new failure modes were generated after the specimens exposed to the elevated temperatures: splitting failure and bottom crushing, and the ultimate bearing capacity of the specimens with bottom crushing is the lowest. The ductility of circular specimens increases with the increases of column height. When the elevated temperature duration reaches 50 min, the plasticity of the specimens basically subside. The ultimate bearing capacity of the timber columns decreases with the increase of the elevated temperature duration and the maximum reduction is about 60% percent.
期刊介绍:
Wood Research publishes original papers aimed at recent advances in all branches of wood science (biology, chemistry, wood physics and mechanics, mechanical and chemical processing etc.). Submission of the manuscript implies that it has not been published before and it is not under consideration for publication elsewhere.