因夹渣而被拒绝的短轴

{"title":"因夹渣而被拒绝的短轴","authors":"","doi":"10.31399/asm.fach.process.c0047118","DOIUrl":null,"url":null,"abstract":"\n An automobile manufacturer rejected several 1035 steel stub axles because of what appeared to be short longitudinal cracks in the surfaces of the pins. The cracks were found when six axles were examined for defects by magnetic-particle inspection. However, metallographic examination showed that these lines were not cracks but slag inclusions at and immediately below the surface. Analysis (visual inspection, metallographic examination, and 100x/500x magnetic-particle inspection) supported the conclusions that the inclusions consisted of pieces of fireclay from channel brick that were flushed into the ingot mold. Although no true cracks were present, rejection of the stub axles was nevertheless justified. Slag streaks could reduce the strength of the stub axles and lead to the formation of fatigue fractures during operation. No recommendations were made.","PeriodicalId":294593,"journal":{"name":"ASM Failure Analysis Case Histories: Processing Errors and Defects","volume":"41 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"2019-06-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Stub Axles That Were Rejected Because of Slag Inclusions\",\"authors\":\"\",\"doi\":\"10.31399/asm.fach.process.c0047118\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"\\n An automobile manufacturer rejected several 1035 steel stub axles because of what appeared to be short longitudinal cracks in the surfaces of the pins. The cracks were found when six axles were examined for defects by magnetic-particle inspection. However, metallographic examination showed that these lines were not cracks but slag inclusions at and immediately below the surface. Analysis (visual inspection, metallographic examination, and 100x/500x magnetic-particle inspection) supported the conclusions that the inclusions consisted of pieces of fireclay from channel brick that were flushed into the ingot mold. Although no true cracks were present, rejection of the stub axles was nevertheless justified. Slag streaks could reduce the strength of the stub axles and lead to the formation of fatigue fractures during operation. No recommendations were made.\",\"PeriodicalId\":294593,\"journal\":{\"name\":\"ASM Failure Analysis Case Histories: Processing Errors and Defects\",\"volume\":\"41 1\",\"pages\":\"0\"},\"PeriodicalIF\":0.0000,\"publicationDate\":\"2019-06-01\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"ASM Failure Analysis Case Histories: Processing Errors and Defects\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.31399/asm.fach.process.c0047118\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"ASM Failure Analysis Case Histories: Processing Errors and Defects","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.31399/asm.fach.process.c0047118","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 0

摘要

一家汽车制造商拒绝了几个1035钢短轴,因为销的表面似乎有短的纵向裂缝。这些裂纹是在对6个轴进行磁粉探伤时发现的。然而,金相检查表明,这些线条不是裂纹,而是在表面及其以下的渣夹杂物。分析(目视检查、金相检查和100倍/500倍磁粉检查)支持这样的结论:内含物是由冲进铸锭模具的槽砖的粘土块组成的。虽然没有真正的裂缝存在,拒绝短轴仍然是合理的。在运行过程中,渣条会降低短轴的强度,导致疲劳断裂的形成。没有提出任何建议。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
Stub Axles That Were Rejected Because of Slag Inclusions
An automobile manufacturer rejected several 1035 steel stub axles because of what appeared to be short longitudinal cracks in the surfaces of the pins. The cracks were found when six axles were examined for defects by magnetic-particle inspection. However, metallographic examination showed that these lines were not cracks but slag inclusions at and immediately below the surface. Analysis (visual inspection, metallographic examination, and 100x/500x magnetic-particle inspection) supported the conclusions that the inclusions consisted of pieces of fireclay from channel brick that were flushed into the ingot mold. Although no true cracks were present, rejection of the stub axles was nevertheless justified. Slag streaks could reduce the strength of the stub axles and lead to the formation of fatigue fractures during operation. No recommendations were made.
求助全文
通过发布文献求助,成功后即可免费获取论文全文。 去求助
来源期刊
自引率
0.00%
发文量
0
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
确定
请完成安全验证×
copy
已复制链接
快去分享给好友吧!
我知道了
右上角分享
点击右上角分享
0
联系我们:info@booksci.cn Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。 Copyright © 2023 布克学术 All rights reserved.
京ICP备2023020795号-1
ghs 京公网安备 11010802042870号
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术官方微信