{"title":"直齿齿轮的剥落故障","authors":"Lester E. Alban","doi":"10.31399/asm.fach.modes.c9001502","DOIUrl":null,"url":null,"abstract":"\n A portion of two large spur tooth bull gears made from 4147H Cr-Mo alloy steel that had spalling teeth was submitted for evaluation. The gears were taken from a final drive wheel reduction unit of a very large open-pit mining truck. The parts had met the material and initial heat treat hardening specifications. The mode of failure was tooth profile spalling. By definition, spalling originates at a case/core interface or at the juncture of a hardened/nonhardened area. The cause of this failure was either insufficient or no induction-hardened case along the active profile. The cause was activated by a nonfunctioning induction hardening coil that did not or was not allowed to harden the midprofile of several teeth.","PeriodicalId":231268,"journal":{"name":"ASM Failure Analysis Case Histories: Failure Modes and Mechanisms","volume":"24 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"2019-06-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Spalling Failure of a Spur Gear\",\"authors\":\"Lester E. Alban\",\"doi\":\"10.31399/asm.fach.modes.c9001502\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"\\n A portion of two large spur tooth bull gears made from 4147H Cr-Mo alloy steel that had spalling teeth was submitted for evaluation. The gears were taken from a final drive wheel reduction unit of a very large open-pit mining truck. The parts had met the material and initial heat treat hardening specifications. The mode of failure was tooth profile spalling. By definition, spalling originates at a case/core interface or at the juncture of a hardened/nonhardened area. The cause of this failure was either insufficient or no induction-hardened case along the active profile. The cause was activated by a nonfunctioning induction hardening coil that did not or was not allowed to harden the midprofile of several teeth.\",\"PeriodicalId\":231268,\"journal\":{\"name\":\"ASM Failure Analysis Case Histories: Failure Modes and Mechanisms\",\"volume\":\"24 1\",\"pages\":\"0\"},\"PeriodicalIF\":0.0000,\"publicationDate\":\"2019-06-01\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"ASM Failure Analysis Case Histories: Failure Modes and Mechanisms\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.31399/asm.fach.modes.c9001502\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"ASM Failure Analysis Case Histories: Failure Modes and Mechanisms","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.31399/asm.fach.modes.c9001502","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
A portion of two large spur tooth bull gears made from 4147H Cr-Mo alloy steel that had spalling teeth was submitted for evaluation. The gears were taken from a final drive wheel reduction unit of a very large open-pit mining truck. The parts had met the material and initial heat treat hardening specifications. The mode of failure was tooth profile spalling. By definition, spalling originates at a case/core interface or at the juncture of a hardened/nonhardened area. The cause of this failure was either insufficient or no induction-hardened case along the active profile. The cause was activated by a nonfunctioning induction hardening coil that did not or was not allowed to harden the midprofile of several teeth.