{"title":"Metal powder composite based on 316L stainless steel bimodal powder","authors":"N. Toropkov, E. Glazkova, N. Rodkevich, A. Pervikov, M. Lerner, S. Muzhetskaya, S. Ghyngazov","doi":"10.1063/1.5132233","DOIUrl":null,"url":null,"abstract":"Metal powder composites for Powder injection molding (PIM) technology have been investigated. 316L stainless steel bimodal powder, obtained by electric explosion of the wire and multicomponent binder comprising PMMA, PE-LD and Viscowax were used to obtain feedstocks. The effect of PMMA content in the binder on the properties of feedstocks and sintered parts has been studied. As the PMMA content increases, the molding temperature of the parts rises from 140 to 200°C, the strength of the “green” and “brow” parts increases as well. The optimal PMMA content in the binder has been found to be 15–20 vol %. “Brown” samples sintered in vacuum at 1300°C exhibit shrinkage up to 23% and the samples density reaches 0.98 TD. Samples of feedstocks were characterized by TEM, SEM, DSC-TG methods.Metal powder composites for Powder injection molding (PIM) technology have been investigated. 316L stainless steel bimodal powder, obtained by electric explosion of the wire and multicomponent binder comprising PMMA, PE-LD and Viscowax were used to obtain feedstocks. The effect of PMMA content in the binder on the properties of feedstocks and sintered parts has been studied. As the PMMA content increases, the molding temperature of the parts rises from 140 to 200°C, the strength of the “green” and “brow” parts increases as well. The optimal PMMA content in the binder has been found to be 15–20 vol %. “Brown” samples sintered in vacuum at 1300°C exhibit shrinkage up to 23% and the samples density reaches 0.98 TD. Samples of feedstocks were characterized by TEM, SEM, DSC-TG methods.","PeriodicalId":20637,"journal":{"name":"PROCEEDINGS OF THE INTERNATIONAL CONFERENCE ON ADVANCED MATERIALS WITH HIERARCHICAL STRUCTURE FOR NEW TECHNOLOGIES AND RELIABLE STRUCTURES 2019","volume":null,"pages":null},"PeriodicalIF":0.0000,"publicationDate":"2019-11-19","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"PROCEEDINGS OF THE INTERNATIONAL CONFERENCE ON ADVANCED MATERIALS WITH HIERARCHICAL STRUCTURE FOR NEW TECHNOLOGIES AND RELIABLE STRUCTURES 2019","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.1063/1.5132233","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 0

Abstract

Metal powder composites for Powder injection molding (PIM) technology have been investigated. 316L stainless steel bimodal powder, obtained by electric explosion of the wire and multicomponent binder comprising PMMA, PE-LD and Viscowax were used to obtain feedstocks. The effect of PMMA content in the binder on the properties of feedstocks and sintered parts has been studied. As the PMMA content increases, the molding temperature of the parts rises from 140 to 200°C, the strength of the “green” and “brow” parts increases as well. The optimal PMMA content in the binder has been found to be 15–20 vol %. “Brown” samples sintered in vacuum at 1300°C exhibit shrinkage up to 23% and the samples density reaches 0.98 TD. Samples of feedstocks were characterized by TEM, SEM, DSC-TG methods.Metal powder composites for Powder injection molding (PIM) technology have been investigated. 316L stainless steel bimodal powder, obtained by electric explosion of the wire and multicomponent binder comprising PMMA, PE-LD and Viscowax were used to obtain feedstocks. The effect of PMMA content in the binder on the properties of feedstocks and sintered parts has been studied. As the PMMA content increases, the molding temperature of the parts rises from 140 to 200°C, the strength of the “green” and “brow” parts increases as well. The optimal PMMA content in the binder has been found to be 15–20 vol %. “Brown” samples sintered in vacuum at 1300°C exhibit shrinkage up to 23% and the samples density reaches 0.98 TD. Samples of feedstocks were characterized by TEM, SEM, DSC-TG methods.
基于316L不锈钢双峰粉末的金属粉末复合材料
研究了用于粉末注射成型(PIM)技术的金属粉末复合材料。以电爆制得的316L不锈钢双峰粉末和由PMMA、PE-LD和粘胶组成的多组分粘结剂为原料。研究了粘结剂中PMMA含量对原料性能和烧结件性能的影响。随着PMMA含量的增加,零件的成型温度从140℃上升到200℃,“绿”件和“眉”件的强度也有所增加。粘结剂中PMMA的最佳含量为15-20 vol %。在1300°C真空烧结的“棕色”样品收缩率高达23%,样品密度达到0.98 TD。采用TEM、SEM、DSC-TG等方法对原料进行表征。研究了用于粉末注射成型(PIM)技术的金属粉末复合材料。以电爆制得的316L不锈钢双峰粉末和由PMMA、PE-LD和粘胶组成的多组分粘结剂为原料。研究了粘结剂中PMMA含量对原料性能和烧结件性能的影响。随着PMMA含量的增加,零件的成型温度从140℃上升到200℃,“绿”件和“眉”件的强度也有所增加。粘结剂中PMMA的最佳含量为15-20 vol %。在1300°C真空烧结的“棕色”样品收缩率高达23%,样品密度达到0.98 TD。采用TEM、SEM、DSC-TG等方法对原料进行表征。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
求助全文
约1分钟内获得全文 求助全文
来源期刊
自引率
0.00%
发文量
0
文献相关原料
公司名称 产品信息 采购帮参考价格
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
确定
请完成安全验证×
copy
已复制链接
快去分享给好友吧!
我知道了
右上角分享
点击右上角分享
0
联系我们:info@booksci.cn Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。 Copyright © 2023 布克学术 All rights reserved.
京ICP备2023020795号-1
ghs 京公网安备 11010802042870号
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术官方微信