{"title":"Characterization of deposit layers formed on grey cast iron","authors":"M. Gwoździk","doi":"10.31648/ts.7896","DOIUrl":null,"url":null,"abstract":"This paper presents the results of diagnostic examinations conducted on the water pipe made of grey cast iron that were operated in conditions for 260 thousand hours. The tube was exposed in a soil. The phase composition of the deposit layers formed on both sides of the tube walls (outside and inside) was examined using optical and confocal microscopy and X-ray diffraction. The obtained XRD test results showed that mainly -FeOOH) and γ-FeOOH is formed on the inside of the pipe wall. In turn, on the outside, in addition to the above-mentioned compounds, also SiO2 is formed. The results of these examinations have shown a higher degradation of pipe on the outer side. The arithmetic mean deviation of the profile from the mean line was 6.23 µm and 8.07 µm for the inner and outer side of the pipe wall, respectively. The work demonstrates the usefulness of material science, especially X-ray structure, topography and surface studies, in characterizing the degradation processes of layers formed on gray cast iron exploited in the water supply industry.","PeriodicalId":41669,"journal":{"name":"Archives for Technical Sciences","volume":null,"pages":null},"PeriodicalIF":0.2000,"publicationDate":"2022-09-05","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"Archives for Technical Sciences","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.31648/ts.7896","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q4","JCRName":"ENGINEERING, GEOLOGICAL","Score":null,"Total":0}
引用次数: 0

Abstract

This paper presents the results of diagnostic examinations conducted on the water pipe made of grey cast iron that were operated in conditions for 260 thousand hours. The tube was exposed in a soil. The phase composition of the deposit layers formed on both sides of the tube walls (outside and inside) was examined using optical and confocal microscopy and X-ray diffraction. The obtained XRD test results showed that mainly -FeOOH) and γ-FeOOH is formed on the inside of the pipe wall. In turn, on the outside, in addition to the above-mentioned compounds, also SiO2 is formed. The results of these examinations have shown a higher degradation of pipe on the outer side. The arithmetic mean deviation of the profile from the mean line was 6.23 µm and 8.07 µm for the inner and outer side of the pipe wall, respectively. The work demonstrates the usefulness of material science, especially X-ray structure, topography and surface studies, in characterizing the degradation processes of layers formed on gray cast iron exploited in the water supply industry.
灰口铸铁上沉积层的表征
本文介绍了灰口铸铁水管在26万小时运行条件下的诊断检测结果。管子暴露在泥土里。利用光学共聚焦显微镜和x射线衍射检查了在管壁两侧(内外)形成的沉积层的相组成。所得XRD测试结果表明,主要是在管壁内侧形成了 -FeOOH)和γ-FeOOH。反过来,在外部,除了上述化合物外,也形成了SiO2。这些试验结果表明,管道外侧的劣化程度较高。管壁内外廓线与均线的算术平均偏差分别为6.23µm和8.07µm。这项工作证明了材料科学,特别是x射线结构、形貌和表面研究,在描述供水工业中使用的灰铸铁层形成的降解过程方面的有用性。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
求助全文
约1分钟内获得全文 求助全文
来源期刊
Archives for Technical Sciences
Archives for Technical Sciences ENGINEERING, GEOLOGICAL-
自引率
0.00%
发文量
10
文献相关原料
公司名称 产品信息 采购帮参考价格
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
确定
请完成安全验证×
copy
已复制链接
快去分享给好友吧!
我知道了
右上角分享
点击右上角分享
0
联系我们:info@booksci.cn Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。 Copyright © 2023 布克学术 All rights reserved.
京ICP备2023020795号-1
ghs 京公网安备 11010802042870号
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术官方微信