{"title":"Broken Milling Machine Arbors Made of 16 Mn Cr 5 E","authors":"Gudrun Urban","doi":"10.31399/asm.fach.machtools.c9001155","DOIUrl":null,"url":null,"abstract":"\n Milling machine arbors were inserted with satellite spindles having a maximum speed of 1500 rpm, and broke out between the groove and the flange. The appearance of the fracture surface was the same on both arbors. The pronounced scan lines characterized the fractures as fatigue fractures. The appearance of the fracture in the arbors indicated ductile fatigue fracture which had its origin in the radii between groove and flange. These radii of 0.15 and 0.2 mm were too small for the load on the milling machine. In addition there were grooves at the base of the radii which had an unfavorable effect on the life of the component by acting as notches with their resulting stress concentration. Considering the great hardness of the case, the small radii would have been critical even without grooves. Measures were taken so that the critical radius of the milling machine was increased and the surface roughness measured more precisely.","PeriodicalId":446028,"journal":{"name":"ASM Failure Analysis Case Histories: Machine Tools and Manufacturing Equipment","volume":"2 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"2019-06-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"ASM Failure Analysis Case Histories: Machine Tools and Manufacturing Equipment","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.31399/asm.fach.machtools.c9001155","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 0

Abstract

Milling machine arbors were inserted with satellite spindles having a maximum speed of 1500 rpm, and broke out between the groove and the flange. The appearance of the fracture surface was the same on both arbors. The pronounced scan lines characterized the fractures as fatigue fractures. The appearance of the fracture in the arbors indicated ductile fatigue fracture which had its origin in the radii between groove and flange. These radii of 0.15 and 0.2 mm were too small for the load on the milling machine. In addition there were grooves at the base of the radii which had an unfavorable effect on the life of the component by acting as notches with their resulting stress concentration. Considering the great hardness of the case, the small radii would have been critical even without grooves. Measures were taken so that the critical radius of the milling machine was increased and the surface roughness measured more precisely.
破碎铣床支架由16mn Cr 5e制成
铣床主轴插入卫星主轴,最大转速为1500转/分,并在槽和法兰之间断裂。两根木杆的断口形貌相同。明显的扫描线特征为疲劳断裂。其断口表现为延性疲劳断裂,起源于槽口与法兰之间的半径处。这些0.15和0.2毫米的半径对于铣床上的负载来说太小了。此外,在半径的底部有凹槽,这对部件的寿命有不利的影响,因为它们作为缺口产生应力集中。考虑到高硬度的情况下,小半径将是至关重要的,即使没有凹槽。采取措施,提高了铣床的临界半径,提高了表面粗糙度的测量精度。
本文章由计算机程序翻译,如有差异,请以英文原文为准。
求助全文
约1分钟内获得全文 求助全文
来源期刊
自引率
0.00%
发文量
0
×
引用
GB/T 7714-2015
复制
MLA
复制
APA
复制
导出至
BibTeX EndNote RefMan NoteFirst NoteExpress
×
提示
您的信息不完整,为了账户安全,请先补充。
现在去补充
×
提示
您因"违规操作"
具体请查看互助需知
我知道了
×
提示
确定
请完成安全验证×
copy
已复制链接
快去分享给好友吧!
我知道了
右上角分享
点击右上角分享
0
联系我们:info@booksci.cn Book学术提供免费学术资源搜索服务,方便国内外学者检索中英文文献。致力于提供最便捷和优质的服务体验。 Copyright © 2023 布克学术 All rights reserved.
京ICP备2023020795号-1
ghs 京公网安备 11010802042870号
Book学术文献互助
Book学术文献互助群
群 号:481959085
Book学术官方微信