{"title":"某电厂锅炉水冷壁管失效分析","authors":"A. El-Batahgy, W. Metwally","doi":"10.31399/asm.fach.power.c9001709","DOIUrl":null,"url":null,"abstract":"\n Several waterwall tubes in a power station boiler failed after ten years of service. The boiler is a suspension type equipped with 30 IK boxes where retractable soot blowers are inserted to clean the inside of the boiler using high-pressure steam. The tubes, which operate at 693 deg F (367 deg C) and 2935 psi (20.5 MPa), failed near the IK boxes as a result of thermal fatigue. Thermal fatigue damage was accelerated by repetitive exposure to water droplets from the soot blower and the associated rapid cooling.","PeriodicalId":107406,"journal":{"name":"ASM Failure Analysis Case Histories: Power Generating Equipment","volume":null,"pages":null},"PeriodicalIF":0.0000,"publicationDate":"2019-06-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":"{\"title\":\"Failure Analysis of Boiler Water Wall-Tubes at a Power Generation Plant\",\"authors\":\"A. El-Batahgy, W. Metwally\",\"doi\":\"10.31399/asm.fach.power.c9001709\",\"DOIUrl\":null,\"url\":null,\"abstract\":\"\\n Several waterwall tubes in a power station boiler failed after ten years of service. The boiler is a suspension type equipped with 30 IK boxes where retractable soot blowers are inserted to clean the inside of the boiler using high-pressure steam. The tubes, which operate at 693 deg F (367 deg C) and 2935 psi (20.5 MPa), failed near the IK boxes as a result of thermal fatigue. Thermal fatigue damage was accelerated by repetitive exposure to water droplets from the soot blower and the associated rapid cooling.\",\"PeriodicalId\":107406,\"journal\":{\"name\":\"ASM Failure Analysis Case Histories: Power Generating Equipment\",\"volume\":null,\"pages\":null},\"PeriodicalIF\":0.0000,\"publicationDate\":\"2019-06-01\",\"publicationTypes\":\"Journal Article\",\"fieldsOfStudy\":null,\"isOpenAccess\":false,\"openAccessPdf\":\"\",\"citationCount\":\"0\",\"resultStr\":null,\"platform\":\"Semanticscholar\",\"paperid\":null,\"PeriodicalName\":\"ASM Failure Analysis Case Histories: Power Generating Equipment\",\"FirstCategoryId\":\"1085\",\"ListUrlMain\":\"https://doi.org/10.31399/asm.fach.power.c9001709\",\"RegionNum\":0,\"RegionCategory\":null,\"ArticlePicture\":[],\"TitleCN\":null,\"AbstractTextCN\":null,\"PMCID\":null,\"EPubDate\":\"\",\"PubModel\":\"\",\"JCR\":\"\",\"JCRName\":\"\",\"Score\":null,\"Total\":0}","platform":"Semanticscholar","paperid":null,"PeriodicalName":"ASM Failure Analysis Case Histories: Power Generating Equipment","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.31399/asm.fach.power.c9001709","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
Failure Analysis of Boiler Water Wall-Tubes at a Power Generation Plant
Several waterwall tubes in a power station boiler failed after ten years of service. The boiler is a suspension type equipped with 30 IK boxes where retractable soot blowers are inserted to clean the inside of the boiler using high-pressure steam. The tubes, which operate at 693 deg F (367 deg C) and 2935 psi (20.5 MPa), failed near the IK boxes as a result of thermal fatigue. Thermal fatigue damage was accelerated by repetitive exposure to water droplets from the soot blower and the associated rapid cooling.