Moamin I. ISSA, Marwah Ismael ABDULAZEEZ, Abdalbseet A. FATALLA
{"title":"Effect of adhesive primer application on shear bond strength of self-adhesive cement to tooth structure and two different CAD/CAM milled blocks","authors":"Moamin I. ISSA, Marwah Ismael ABDULAZEEZ, Abdalbseet A. FATALLA","doi":"10.4322/bds.2023.e3978","DOIUrl":null,"url":null,"abstract":"Objective: This study was conducted to evaluate the influence of the G-CEM ONE adhesive enhancing primer on the shear bond strength of self-adhesive resin cement (G-CEM ONE) to both tooth structure and two different CAD/ CAM blocks (GC Initial LiSi and Cerasmart 270). Material and Methods: Forty specimens (cylindrical-shaped, 5 mm in diameter and height) were milled from both CAD/CAM blocks (20 specimens from each block type). Forty sound upper premolars were sectioned to the level of peripheral dentin, then randomly divided into four groups (n = 10): A1: GC Initial LiSi without adhesive enhancing primer; B1: Cerasmart 270 without adhesive enhancing primer; A2: GC Initial LiSi with adhesive enhancing primer; B2: Cerasmart 270 group with adhesive enhancing primer application. The CAD/CAM blocks were cemented on teeth using a self-adhesive resin cement (G-cem one). The shear bond strength was assessed using a computerized universal testing machine. A digital microscope was used to study the mode of failure. The shear bond strength values data were analyzed statistically using paired t-test and independent t-test at the significance level of (0.05). Results: A significant difference was shown in the shear bond strength values among groups (P =0.000). The highest shear bond strength value was revealed in group A2, while group B1 exhibited the lowest shear bond strength value. Conclusion: Using the adhesive enhancing primer on the tooth’s surface improved the resin cement’s bond strength to CAD/CAM blocks. Additionally, GC Initial LiSi exhibited higher bond strength than Cerasmart 270, with or without the primer. KEYWORDS Adhesive; CAD/CAM; Dentin; Resin cement; Shear strength.","PeriodicalId":37577,"journal":{"name":"Brazilian Dental Science","volume":"32 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"2023-01-01","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"Brazilian Dental Science","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.4322/bds.2023.e3978","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"Q3","JCRName":"Dentistry","Score":null,"Total":0}
引用次数: 0
Abstract
Objective: This study was conducted to evaluate the influence of the G-CEM ONE adhesive enhancing primer on the shear bond strength of self-adhesive resin cement (G-CEM ONE) to both tooth structure and two different CAD/ CAM blocks (GC Initial LiSi and Cerasmart 270). Material and Methods: Forty specimens (cylindrical-shaped, 5 mm in diameter and height) were milled from both CAD/CAM blocks (20 specimens from each block type). Forty sound upper premolars were sectioned to the level of peripheral dentin, then randomly divided into four groups (n = 10): A1: GC Initial LiSi without adhesive enhancing primer; B1: Cerasmart 270 without adhesive enhancing primer; A2: GC Initial LiSi with adhesive enhancing primer; B2: Cerasmart 270 group with adhesive enhancing primer application. The CAD/CAM blocks were cemented on teeth using a self-adhesive resin cement (G-cem one). The shear bond strength was assessed using a computerized universal testing machine. A digital microscope was used to study the mode of failure. The shear bond strength values data were analyzed statistically using paired t-test and independent t-test at the significance level of (0.05). Results: A significant difference was shown in the shear bond strength values among groups (P =0.000). The highest shear bond strength value was revealed in group A2, while group B1 exhibited the lowest shear bond strength value. Conclusion: Using the adhesive enhancing primer on the tooth’s surface improved the resin cement’s bond strength to CAD/CAM blocks. Additionally, GC Initial LiSi exhibited higher bond strength than Cerasmart 270, with or without the primer. KEYWORDS Adhesive; CAD/CAM; Dentin; Resin cement; Shear strength.
期刊介绍:
The Journal BRAZILIAN DENTAL SCIENCE is a trimonthly scientific publication of the Institute of Science and Technology of São José dos Campos - UNESP. MISSION - To disseminate and promote the interchange of scientific information amongst the national and international dental community, by means of basic and applied research.