{"title":"Performance Evaluation of Structural Lightweight Concrete Using Jhama Brick as a Partial Replacement of Coarse Aggregate","authors":"M. Haque","doi":"10.36937/cebacom.2022.5676","DOIUrl":null,"url":null,"abstract":"Through the ancient time structural lightweight concrete has been used successfully all over the world due to having its pleasant property of reducing dead load of multi-storied buildings which is very much important for high rising structures. This research represents the experimental works on the structural lightweight concrete to observe the cost and the physical properties using jhama brick (also known as over burnt brick) chips as partial replacement of coarse aggregate. For producing C-35 grade concrete, jhama brick chips was used for the partial replacement of coarse aggregate by 0%, 5%, 10%, 15%, 20%, 25%, and 30% weight of coarse aggregate. For this purpose, 21 sets of cylinders (100 mm x 200 mm) were prepared. Slump tests were carried out for each mix in the fresh state and 3, 7 and 28 days of compressive strength tests were also performed in the hardened state. The 28-days compressive strength of concrete with 0%, 5%, 10%, 15%, 20%, 25%, and 30% replacement of jhama brick chips were 37.12, 36.37, 34.23, 33.01, 30.89, 30.50, and 21.98 MPa respectively. The unit weight of concrete with 0%, 5%, 10%, 15%, 20%, 25%, and 30% replacement of jhama brick chips after 28-days curing were found 2409.3, 2379.2, 2286.9, 2230.2, 2197.0, 2104.1, and 2094.9 kg/m3 respectively. According to ASTM C 330, the compressive strength of concrete with jhama brick chips up to 25% of coarse aggregate fulfilled its requirements.","PeriodicalId":343973,"journal":{"name":"Journal of Cement Based Composites","volume":"46 1","pages":"0"},"PeriodicalIF":0.0000,"publicationDate":"2022-09-02","publicationTypes":"Journal Article","fieldsOfStudy":null,"isOpenAccess":false,"openAccessPdf":"","citationCount":"0","resultStr":null,"platform":"Semanticscholar","paperid":null,"PeriodicalName":"Journal of Cement Based Composites","FirstCategoryId":"1085","ListUrlMain":"https://doi.org/10.36937/cebacom.2022.5676","RegionNum":0,"RegionCategory":null,"ArticlePicture":[],"TitleCN":null,"AbstractTextCN":null,"PMCID":null,"EPubDate":"","PubModel":"","JCR":"","JCRName":"","Score":null,"Total":0}
引用次数: 0
Abstract
Through the ancient time structural lightweight concrete has been used successfully all over the world due to having its pleasant property of reducing dead load of multi-storied buildings which is very much important for high rising structures. This research represents the experimental works on the structural lightweight concrete to observe the cost and the physical properties using jhama brick (also known as over burnt brick) chips as partial replacement of coarse aggregate. For producing C-35 grade concrete, jhama brick chips was used for the partial replacement of coarse aggregate by 0%, 5%, 10%, 15%, 20%, 25%, and 30% weight of coarse aggregate. For this purpose, 21 sets of cylinders (100 mm x 200 mm) were prepared. Slump tests were carried out for each mix in the fresh state and 3, 7 and 28 days of compressive strength tests were also performed in the hardened state. The 28-days compressive strength of concrete with 0%, 5%, 10%, 15%, 20%, 25%, and 30% replacement of jhama brick chips were 37.12, 36.37, 34.23, 33.01, 30.89, 30.50, and 21.98 MPa respectively. The unit weight of concrete with 0%, 5%, 10%, 15%, 20%, 25%, and 30% replacement of jhama brick chips after 28-days curing were found 2409.3, 2379.2, 2286.9, 2230.2, 2197.0, 2104.1, and 2094.9 kg/m3 respectively. According to ASTM C 330, the compressive strength of concrete with jhama brick chips up to 25% of coarse aggregate fulfilled its requirements.
从古至今,结构轻量化混凝土由于其降低多层建筑自重的优良性能,在世界范围内得到了成功的应用,这对高层建筑具有重要意义。本研究是对结构轻量化混凝土进行试验研究,以观察用焦化砖(也称为过烧砖)碎片部分替代粗集料的成本和物理性能。为生产C-35级混凝土,采用jhama砖屑,用0%、5%、10%、15%、20%、25%、30%重量的粗骨料部分替代粗骨料。为此,制备了21组圆柱体(100 mm x 200 mm)。在新鲜状态下进行了坍落度试验,在硬化状态下进行了3、7和28天的抗压强度试验。替换量为0%、5%、10%、15%、20%、25%、30%的碎块混凝土28天抗压强度分别为37.12、36.37、34.23、33.01、30.89、30.50、21.98 MPa。养护28 d后,砌块置换率为0%、5%、10%、15%、20%、25%、30%的混凝土单位重量分别为2409.3、2379.2、2286.9、2230.2、2197.0、2104.1、2094.9 kg/m3。根据ASTM C 330标准,含粗骨料25%的jhama砖片的混凝土抗压强度达到要求。